Pearl chrome plating auto interior parts Management
Pearl nickel is widely used in automotive interior parts because the products plated are non-reflective and produce diffuse reflection when the strong light is directly reflected, which is not harsh to the eyes, feels soft and comfortable, and has no fingerprints.
At present, the market is common for short-acting sand and long-acting sand, because the long-acting sand is more widely used, we will talk about the control skills of long-acting sand.
I. Control of the main salt composition
1, the main salt ingredients are mainly nickel sulfate, nickel chloride, boric acid, the content of these ingredients must be controlled in the process range on the upper side, because the main ingredients of nickel pearl will be brought in and out of the drop is more obvious.
2、Prepare a high concentration of make-up liquid, must be pre-electrolyzed well to avoid the impact of impurities.
II. Focus on the circulation pump
Must ensure that the circulation pump does not leak, otherwise it will have a great impact on the long-term performance of the pearl nickel plating solution. So the pipeline of the circulation pump must ensure its sealing.
Pearl chrome plating auto interior parts Management
III. Carbon treatment plating solution should be thorough
Generally speaking, if the pearl nickel is well maintained, only general carbon treatment is needed, if the disorder is serious, potassium permanganate - hydrogen peroxide - carbon treatment is needed.
1, after the carbon must be laboratory test piece analysis of carbon treatment is complete? Only if the carbon treatment is complete, the test piece can be added to adjust the amount.
2, toner is also a very critical issue, must buy high-quality toner, otherwise the impact on the pearl nickel plating solution is extremely huge, before a chemical reagent factory AR toner on the entire batch out of order, resulting in many plating factory pearl nickel potion can not be adjusted over a long period of time.
Ⅳ. pearl nickel color is the key
The factory I manage has always been a dedicated post, select people who work seriously and are sensitive to color to take up this important position. Requirements are as follows.
1, control the production schedule, to ensure that the pearl nickel and chromium sets are not backlogged, to prevent peeling between the layers
2, to ensure that the color of each cylinder to be made out of the eyes, and 30 minutes to a color plate.
3、Copy the color sample, the sample shall not be touched by hand to ensure the validity of the sample
4、To pay attention to the difference between high electric area & low electric area, adjust the process parameters appropriately
Ⅴ. Focus on the control of pearl nickel layer bonding problem
1, the aforementioned control of pearl nickel production schedule, shall not cause backlog.
2, pearl nickel activation is best not to use the traditional acid activation, the use of pre-plating nickel instead of activation, so as to effectively ensure the pearl nickel layer and the front of the nickel layer bonding.
3, chromium activation before, it is best to take the energized chromium activation.
Above article introduced Pearl chrome plating auto interior parts Management.