Common faults and correction methods of decorative chrome plating
Insufficient light
a) Low temperature or high current density
b) Low sulfate content
c) High trivalent chromium
d) High content of iron impurities
a) heat up, check whether the current is within the process range
b) Analysis supplement
c) Large anode, small cathode electrolysis
d) Electrolysis with ion exchange or diaphragm
poor coverage
a) High temperature and low current density
b) high sulfuric acid content,
c) Insufficient trivalent chromium
d) There are many impurities of zinc, copper, and iron
a) lower, check whether the current is within the process range
b) use BaCO3 after analysis to remove part of the sulfate radical;
c) Large cathode, small anode electrolysis
d) Ion exchange or diaphragm electrolytic treatment
Local chrome-free layer
a) The holes are not blocked
b) Improper mounting and hanging, resulting in air pockets or poor electrical conductivity
c) The shape of the part is complex and the auxiliary anode is not used
d) Mutual shielding of parts
e) There is oil on the surface of the plated parts
f) The hanger is not insulated
a) plugged with the plastic tube
b) use a hanger instead
c) Choose an appropriate auxiliary anode
d) Fewer hanging parts
e) Reprocessing the plated parts
f) Improve hanger insulation
The chrome layer is peeled off with the nickel layer
a) Incomplete pre-plating treatment
b) The internal stress of the nickel-plated layer is large
a) Strengthen the pre-plating treatment
b) Adjust the nickel plating solution
Black scratches appear when chrome plating on copper-tin alloy coating
a) The solution temperature is low
b) Incomplete pretreatment of chrome plating
c) Power on too fast or too slow
e) The content of tin in the copper-tin alloy is too high
a) raise the temperature
b) Strengthen the pretreatment of chrome plating
c) Improve operation
e) Adjust the copper-tin alloy
Hard chrome plating
Plating peels off
a) Poor pre-plating treatment
b) Power off during the chrome plating process
c) Short preheating time for parts into the groove
d) Too much variation in solution temperature or cathode current density
e) The sulfuric acid content is too high
a) Strengthen the pre-plating treatment
b) When re-chrome plating, carry out anodic treatment or cathode small current activation treatment
c) Extend the warm-up time
d) Strictly control solution temperature and cathode current density
e) Add barium carbonate treatment
Iron castings cannot be plated with chrome,
only hydrogen evolution reaction
a) Excessive etching before plating
b) When anodizing is performed, the graphite is exposed
c) The cathode current density is too low
a) Re-processed and then plated
b) Re-plating after full processing
c) Increase the cathode current density
Rough coating with chromium
a) The cathode current density is too large
b) The distance between the cathode and anode is too close
c) The shape of the part is convex, and the protective cathode is not used
d) Too much sulfate
a) Reduce the cathode current density
b) Relax the distance between cathode and anode
c) Use a suitable protective cathode
d) Add barium carbonate treatment
Visible cracks in the coating or the underlying metal
Steel is stressed when quenched
Temper parts to relieve stress before plating