9 common fault solutions for nickel electroplating
The main defects of nickel electroplating are: poor pretreatment, metal impurities, too little boric acid content, and too low temperature of the plating solution, which will lead to pinholes in the electroplated nickel layer, and the maintenance of the plating solution and the strict control process is the key. Solve the following "nine" major faults, and the basic problems will be controlled.
1) Hemp pit (pinhole)
The pits (pinholes) are the result of organic pollution. Large hemp pits usually indicate that there is oil pollution, which needs to be decomposed and treated with carbon. Poor stirring will not dislodge air bubbles, and pits (pinholes) will form. Wetting agents can be used to reduce their effects.
2) Rough (burr)
Roughness means that the solution is dirty and can be corrected after sufficient filtration. The value is too high and easy to form hydroxide precipitation, which should be controlled; the current density is too high, the anode slime and the added water are impure, and impurities will be generated in severe cases...
3) Low binding force
If the copper coating is not activated to remove the oxide layer, the adhesion between copper and nickel is poor, and the phenomenon of coating peeling will occur. If the current is interrupted, it may cause the nickel coating to peel off; if the temperature is too low, peeling will also occur.
4) The coating is brittle and has poor solderability
When the coating is bent or subjected to a certain degree of wear, the brittleness of the coating is usually revealed, which indicates the presence of organic or heavy metal contamination. Too many additives will increase the organic matter and decomposition products entrained in the coating, which is the main source of organic pollution, which can be treated with activated carbon; heavy metal impurities can be removed by electrolysis and other methods.
5) The coating is dark and uneven in color
Dullness and uneven coloration of the coating indicates metal contamination. Because copper is usually plated first and then nickel is plated, the copper solution carried by people is the main source of pollution. It is important to reduce the copper solution on the hanger to a minimum. In order to eliminate the metal pollution in the nickel plating tank, a corrugated steel plate is used as the cathode, and electrolytic treatment is carried out at a current density of 02-0.5A/dm2. Poor pretreatment, poor bottom coating, too low current density, too low main salt concentration, and poor conductive contact will affect the color of the coating.
6) Coating burnt
Insufficient boric acid, low concentration of metal salts, too low working temperature, too high current density, too high pH value, or insufficient stirring are all possible causes of charring of the coating.
7) Low deposition rate or low current density will result in low deposition rate.
8) The coating is blistered or peeled
Poor pre-plating treatment, long interruption time, organic impurity pollution, too high current density, too low temperature, too high or too low PH value, and serious influence of impurities will cause blistering or peeling.
9) Anode passivation
Insufficient anode activator (nickel chloride), too small anode area and too high current density can lead to anode passivation.