Plastic parts water plating step 1. Remove wax:
After the plastic parts are polished, there is a layer of wax on the surface. In order to ensure the quality after plating, wax removal treatment is required.
Process conditions:
Dewax MK101 10-30ml/L
Temperature 60-75℃ Time 4-7min
Ultrasonic 2-8A
(This process is selected according to the actual situation)
Plastic parts water plating step 2. Degreasing:
Parts are inevitably stained with oil during molding, storage and transportation. In order to ensure the effect of pre-plating treatment, oil removal treatment should be carried out before coarsening.
A. Process conditions:
Hot dip degreasing powder MK111 50g/L
Temperature 50-60℃ Time 2-3min
B. Effect inspection: Check whether the surface of the product after degreasing treatment is hydrophilic, if it is not hydrophilic or not completely hydrophilic, it must be re-tested.
Plastic parts water plating step 3. Roughening
The purpose of roughening is to improve the hydrophilicity of the surface of the part and form an appropriate surface roughness to ensure that the water electroplating has a good bonding force.
A. Roughening process:
Chromic acid 390-410g/L Sulfuric acid 380-410g/L
Temperature 68-70℃ Time 8-15min
Trivalent chromium <15g/L
B. Roughening quality inspection: In addition to requiring the surface to be completely wetted by water, it can also be judged from the appearance. The relationship between the degree of roughening and the surface characteristics is as follows:

Plastic parts water plating step 4, neutralization:
After chemical roughening, neutralization, reduction or acid pickling should be carried out. The purpose is to clean the hexavalent chromium remaining on the surface of the parts to prevent contamination of the dipping solution. ----
Neutralization process:
Hydrochloric acid 40-60ml/L
Hydrazine hydrate (80%) 1-2ml/L
Temperature: Room temperature Time: 1-3min.
Plastic parts water plating step 5, pre-impregnation:
In order to prevent the plastic parts from bringing water into the activation tank, the plastic parts must be pre-soaked before the colloidal palladium is activated.
Pre-soaking process: Hydrochloric acid 50ml/L
Time 0.5-1min Temperature Room temperature.
~~~~~~to be continued~~~~~~