Ⅵ. Colloidal palladium activation:
A layer of catalytically active noble metal layer is formed on the surface of the part, so that the electroless plating can be carried out spontaneously.
A Palladium sinking process: Hydrochloric acid 230-320ml/L
Plastic electroplating activator MK802 3-7ml/L
Stannous chloride 2-6g/L Temperature 25-30℃
Time 2-5min
B Operation notes:
1. Avoid the introduction of hexavalent chromium in the roughening solution. The hexavalent chromium consumes stannous chloride and is reduced to trivalent chromium. This trivalent chromium will significantly reduce the efficiency of the activation solution. When the mass concentration of trivalent chromium exceeds 0.15g When /L, the activation solution becomes invalid.
2. Air stirring cannot be used when preparing the solution.
3. When the mass concentration of stannous chloride in the solution is lower than 0.1g/L, the activation solution will become invalid and should be supplemented before.
Ⅶ,Degumming:
The parts activated by colloidal palladium have colloidal palladium particles adsorbed on the surface, which has no catalytic activity. Because the colloidal divalent tin hydrolyzed gel layer is adsorbed around the palladium particles, it is necessary to make the palladium particles act as a catalytic active center. De-glue the surface of the product.
A Degumming process: sulfuric acid 23-30ml/L
Plastic plating acceleration salt MK805 60-80g/L
PH 0.5-1.5 Temperature 35-55℃ Time 1-3min
B Inspection: After the glue is removed, the surface of the part is uniformly light brown, otherwise it means that the treatment is not good and should be reworked.
Ⅷ, electroless nickel plating:
After the plastic product undergoes strict pre-plating treatment, before the formal decorative electroplating, the surface must be pre-metalized, that is, electroless copper or electroless nickel plating is used to cover the surface with a thin layer of metal, and then electroplating The method of thickening to form the required metal coating with certain physical and chemical properties.
A Chemical nickel process: nickel sulfate 18-27g/L
Sodium hypophosphite 10-15g/L
Plastic chemical nickel MK811C 50-85ml/L
Ammonia water about 15ml/ PH 7.5-8.5
Temperature 33-42℃ Time 6-8min
B Operation note:
1. Strictly prevent the solution from being polluted during production.
2. When adjusting and adding various raw materials, it is not allowed to directly add solid raw materials into the solution, but must be dissolved and filtered before adding an appropriate amount.
3. Filter to remove the solid particles in the solution in time.
Ⅸ, follow-up electroplating:
After the electroless nickel plating is completed, re-plating of scorched copper, acid copper, bright nickel, semi-gloss nickel, bright chromium or chromium replacement as required, and the process conditions are the same as those of metal electroplating.