sunxinzheng2008@163.com    +86-13713943531
enLanguage
Cont

Have any Questions?

+86-13713943531

Jan 10, 2022

Weather Resistance Of Decorative Black Chrome Electroplating For Automobiles

Weather resistance of decorative black chrome electroplating for automobiles

Decorative electroplating products are widely used in radiator grilles, anti-scratch strips, door handles, rearview mirrors, instrument panels, and other automotive interior and exterior decoration areas. With the continuous improvement of customers' aesthetics and the requirements of OEMs for high-end decoration, the traditional bright chrome and satin can no longer be satisfied.


Electroplating black chrome has gradually emerged in China since 2008 because of its shocking new appearance and high-end visual sense. Compared with traditional bright chrome, electroplating black chrome adds Fe, S, and other elements to the chrome plating process layer to form an alloy coating on the surface, thereby producing a black metal appearance effect. Since black chrome plating does not have the self-passivation effect of white chrome and is more brittle, the corrosion resistance is theoretically reduced. In this paper, taking black chrome electroplating on plastic as the research object, the weather resistance of black chrome is studied and analyzed from the aspects of corrosion resistance and aging resistance of parts and vehicles, compared with the traditional bright chrome process.

1)Experimental materials and methods

Electroplating process The electroplating process is: cleaning and pre-etching -> corrosion cleaning - neutralization - pre-dipping - catalysis - cleaning - debonding - chemical plating - pre-plating - acid copper - activation - semi-bright nickel - light nickel / pearl nickel - nickel seal (Microporous)—Black Chrome/Bright Chrome. 3. Test description The test samples are all samples produced according to the normal process except the vehicle exposed parts which are test plates. In order to analyze the influence of the environment on black chromium in detail, the environmental data of the Hainan exposure test site within one year and the temperature, humidity, and irradiance of the test vehicle where the sample is located were recorded.

Explanation of vehicle exposure: The natural exposure of vehicles has always been the most reliable and richest source of information for studying atmospheric natural corrosion. The vehicle exposure test site is located in Qionghai, Hainan, which is far from the marine climate and industrial atmospheric climate, and the environmental corrosion intensity is small. The exterior trim panel is placed on the roof, the interior trim panel is placed on the dashboard, and the exterior trim color panels are cleaned normally every month.


2)Test results and analysis


1. The anti-corrosion performance of black chrome The main factors affecting the anti-corrosion performance of decorative electroplating are the thickness of the coating, the potential difference, the number of micropores/microcracks, and the structure of the coating. The major OEMs have separately stipulated the above indicators, and several performances that affect the anti-corrosion in this test are basically within the range required by the major OEMs. For exterior parts, after 48 hours of CASS test, star pitting corrosion appeared on the surface of black chrome, as shown in Figure 1. After 24 hours of the CASS test of interior parts, there is no obvious change in appearance. The results show that the appearance of bright chrome and black chrome has no obvious difference in the CASS test for 24h; the CASS test for 48h shows that the black chrome is easier to corrode than the bright chrome.

2. Xenon lamp aging resistance of black chrome The 4 groups of black chrome samples are subjected to xenon lamp aging resistance test according to the exterior parts, the irradiance is 0.5W/(m2.nm)@340rnn, the black mark temperature is 65°C, relative The humidity is 65%, no water spray for 108 minutes, and water spray for 12 minutes. Observe at 750 and 1250h respectively, and evaluate the color fastness according to GB/T250-2008.

With the increase of the aging time of the xenon lamp, there is no obvious appearance defect of the coating except that the appearance gloss becomes darker. 3. Natural exposure resistance of black chrome The interior black chrome swatch has no obvious appearance changes, so I won't go into details here. The three exterior trim samples are shown in Figure 3, from left to right are bright chrome, black chrome (light color), and black chrome (dark color). It can be seen from the test board that the surface of bright chrome is still bright, the surface of black chrome (light color) is slightly florid, and the surface of black chrome (dark color) has serious fluorescence, and products similar to tea water stains and rust spots appear and are washed with water. , alkaline detergent, alcohol, etc. cannot be erased, and there is no corrosion phenomenon such as pitting and corrosion pits.

This phenomenon is not reflected in the CASS test and the xenon lamp aging test. The conversion relationship between xenon lamp aging and natural exposure is about 7 times. Natural exposure for 1 year is equivalent to 1251h, which is basically the same as the xenon lamp aging time of 1250 hours. Xenon lamp aging for 1250h does not appear natural exposure. Flowering phenomenon. From the above data, it is shown that light is not the root cause of black chrome blooming. Black chrome alone is resistant to high temperature and natural exposure. The interior temperature is higher than the exterior temperature, but there is no obvious change in appearance, indicating that temperature is not the root cause of the coating blooming. From the analysis of the CASS test, the corrosion resistance of the black chrome alloy layer has decreased, so the comprehensive analysis of temperature, light, humidity, and CASS shows that with the increase of the CASS test, the coating has pitting corrosion, while other factors change the coating No significant change occurred. Therefore, in the natural environment where natural exposure is located, the main reason for the blooming of the coating is that the black chrome coating is oxidized, and the presence of the blackening agent in the coating causes the coating to produce products similar to rust spots and tea stains.

03 point of view

1) The self-plating effect of electroplating black chrome for exterior parts is poorer than that of electroplating bright chrome, and the phenomenon of coating blooming may occur during the normal use of the vehicle, while there is no significant difference between interior parts and bright chrome. 2) High temperature and ultraviolet rays have little effect on the weather resistance of black chrome. 3) The anti-corrosion performance of the electroplated black chrome alloy layer is lower than that of the traditional electroplated bright chrome layer. Electroplating black chrome process is recommended for interior areas. Electroplating black chrome for exterior decoration is recommended to choose a light color to reduce the risk of discoloration and blooming, and according to weather resistance requirements, it is possible to consider adding treatments other than passivation and sealing, such as transparent coating, etc., to improve the decorative and weather resistance of the coating.