Plastic Plating-Nine Common Problems Solutions for Nickel Electroplating
Huizhou City Boluo Tenglong Technology Co., Ltd. wholeheartedly serves you! Mainly engaged in plastic water electroplating processing, accompanying plastic injection molding processing, mold processing and so on!
The main disadvantages of nickel electroplating are: poor pretreatment, metal impurities, too little boric acid content, and too low plating solution temperature will lead to pinholes in the plated nickel layer. The maintenance of the plating solution and strict control process are the key. By solving the following "nine" major faults, the basic problems will be under control.
1)Macheng (pinhole)
Pitted pits (pinholes) are the result of organic pollution. Large pits usually indicate that there is oil pollution that needs to be decomposed and carbon treated. If the stirring is not good, the bubbles cannot be expelled, and pits (pinholes) will be formed. A wetting agent can be used to reduce the influence.
2)Roughness (burr)
Roughness means that the solution is dirty and can be corrected by sufficient filtration. If the value is too high, it will easily form hydroxide precipitates, which should be controlled; if the current density is too high, the anode mud and makeup water are impure and impurities, roughness (burrs) will be produced in severe cases.
3)Low binding power
If the copper plating layer is not activated to remove the oxide layer, the adhesion between copper and nickel will be poor, and the plating layer will be peeled off. If the current is interrupted, it may cause the nickel coating to flake off itself; if the temperature is too low, peeling may also occur.
4)The coating is brittle and has poor solderability
When the coating is bent or subjected to a certain degree of wear, the brittleness of the coating is usually revealed, which indicates the presence of organic matter or heavy metal contamination. Too much additives will increase the amount of organic matter and decomposition products entrained in the coating. It is the main source of organic pollution and can be treated with activated carbon; heavy metal impurities can be removed by electrolysis and other methods.
5)Coating is dark and uneven in color
Dark coating and uneven color indicate metal contamination. Because copper plating is generally carried out first and then nickel plating, the leading copper solution is the main source of pollution. It is important to minimize the copper solution stained on the hangers. In order to eliminate metal pollution in the nickel plating bath, corrugated steel plates are used as the cathode and electrolytically treated at a current density of 02-0.5A/dm2. Poor pretreatment, poor primer coating, too small current density, too low main salt concentration, and poor conductive contact will all affect the color of the coating.
6)coating scorched
Insufficient boric acid, low concentration of metal salts, too low working temperature, too high current density, too high PH value or insufficient stirring are all possible causes of charring of the coating
7)Low deposition rates or low current densities can cause low deposition rates.
8)Blistering or peeling of coating
Poor pre-plating treatment, long intermediate power outage time, organic impurity pollution, excessive current density, too low temperature, too high or too low PH value, and serious influence of impurities may cause foaming or peeling.
9)anodic passivation
Insufficient anode activator (nickel chloride), too small anode area, and too high current density can lead to anode passivation.