Plastic plating-Electrophoretic coating process of ABS plastic plating.
The general technological process of electrophoresis is as follows:
Workpiece pretreatment (deoiling "hot water washing" derusting "cold water washing" phosphating "hot water washing" passivation) "electrophoresis" clean water washing "drying"
1. Deoiling.
The solution is generally thermal alkaline chemical deoiling solution, the temperature is 60 ℃ (steam heating), the time is about 20min.
two.. Hot water washing.
Temperature 60 ℃ (steam heating), time 2min.
3. Rust removal.
Use H2SO4 or HCl, such as hydrochloric acid rust remover, HCl total acidity ≥ 43 points; free acidity > 41 points; add cleaning agent 1.5%; wash 10~20min at room temperature.
4. Cold washing.
Wash 1min with cold water in flow.
5. Phosphating.
Phosphating at medium temperature (phosphating 10min at 60 ℃).
6. Passivation.
With the medicine matched with the phosphating solution, 1~2min can be used at room temperature.
7. Anodic electrophoresis.
The composition of the electrolyte: the mass fraction of solid is 9%-12%, and that of distilled water is 88%-91%.
Voltage: (70 ±10) V; time: 2~2.5min.
Paint temperature: 15 ℃ 35 ℃.
Ph value of paint liquid: 8: 8.5.
In the process of electrophoresis, the current will gradually decrease with the thickening of the paint film, so pay attention to the power outage of the workpiece in and out of the slot.
8. Wash with clean water.
Wash in flowing cold water.
9. Drying.
40~60min can be baked at 165C in the oven.
Apr 10, 2024