Failure causes and troubleshooting in plastic electroplating-electroplating process.
Huizhou Boluo Tenglong Technology Co., Ltd. serves you wholeheartedly! Mainly engaged in plastic hydroelectroplating processing, with plastic injection molding processing, mold processing and so on!
1 Ma Keng (pinhole).
Ma Keng is the result of organic pollution. Large pockets usually indicate oil pollution. If the mixing is bad, the bubbles cannot be expelled, which will form pockmarked holes. Wetting agents can be used to reduce its effect. We usually call small pinholes, which are produced by poor pretreatment, metal impurities, too little boric acid and too low bath temperature. therefore, the maintenance of the plating solution and strict control of the process is the key.
2 rough (burr).
Roughness means that the solution is dirty and can be corrected by full filtration; the formation of hydroxide precipitation when PH is too high should be controlled; if the current density is too high, anode slime and adding water will bring impurities, which will produce rough (burr) when serious.
3The binding force is low.
If the copper coating is not activated to remove the oxidation layer, the adhesion between copper and nickel is poor, and the coating will peel off. If the current is interrupted, it may cause the nickel coating to peel off itself; if the temperature is too low, it will also peel off.
(4) the coating is brittle and poor solderability.
When the coating is bent or worn to a certain extent, the brittleness of the coating is usually revealed, which indicates the existence of organic or heavy metal contamination. Too many additives increase the organic matter and decomposition products in the coating, which is the main source of organic pollution and can be treated with activated carbon, and heavy metal impurities can be removed by electrolysis.
(5) the coating is dark and uneven in color.
The coating is dark and uneven in color, indicating metal pollution. Because copper plating is usually followed by nickel plating, the copper solution brought in is the main source of pollution. It is important to minimize the copper solution in the pendant. In order to remove the metal pollution in the tank, the corrugated steel plate was used as the cathode and electrolyzed under the current density of 0.12~0.50A/d. Poor pretreatment, poor bottom coating, low current density, low concentration of main salt and poor conductive contact will affect the color of the coating.
6 coating burns.
The possible causes of coating burn include insufficient boric acid, low concentration of metal salt, low working temperature, high current density, high PH value or insufficient stirring.
(7) low deposition rate.
Low PH value or low current density will result in low deposition rate.
8 blistering or peeling of the coating.
Blistering or peeling will occur when poor pre-plating treatment, long power cut-off time, organic impurity pollution, too high current density, too low temperature, too high or too low PH value, and serious influence of impurities will occur.
9 anodic passivation.
The anode activator is insufficient, the anode area is too small and the current density is too high.