Chrome coating thickness uniformity

Chrome coating thickness uniformity

The chrome plating layer, especially the chrome plating layer of the gun barrel, has strict requirements on thickness uniformity. Due to the poor dispersion ability of the chrome plating solution, when chrome plating large workpieces, especially hard chrome plating with long plating time and high current, the thicker the chromium layer is deposited, the easier it is to cause uneven current distribution, resulting in problems such as taper, ovality, "dog bone" "Defects in form, etc. In this paper, the effects of anode, internal resistance, trivalent chromium, and other factors on the thickness uniformity of chromium plating layer are introduced.


1 Influence of anode and plating layout


1.1 Anode location


Generally, the uniformity of the thickness of the chrome layer depends on the relationship between the anode and the plated part. Typically, the closer the anode is to the plated part, the more the chrome layer conforms to the plated part's geometry. However, when the outer diameter of the anode and the plated part are not similar, if the distance between the anode and the plated part is increased, the current can be distributed more evenly on the surface of the anode; if the distance between the anode and the plated part is too close, the current distribution will be uneven. . When plating workpieces with outer diameters, the distance between the anode and the plated workpiece should be controlled within the range of 10 to 25 cm. If the anode is too far away from the plated part, the resistance of the solution increases and the power loss increases. The following should be done in operation:


(1) The plated parts with simpler shapes can be closer to the anode; the plated parts with irregular shapes should be as large as possible from the anode.


(2) The plated parts with different sizes cannot be plated in the same tank to avoid serious uneven current distribution.


(3) The distance between the different parts of the plated parts and the anode should be as equal as possible, so that the resistance of the solution can be similar and the current distribution can be uniform.


(4) Position the plated parts (especially the shaft) in their respective "boxes" composed of 4 anodes, so that the current can be evenly distributed on the surface of the plated parts and avoid ovality.


1.2 The anode is too long


The lead alloy anode used for hard chrome plating should be shorter than the plated parts (especially the shaft). The top of the anode is slightly lower than the top of the plated part, and the bottom of the anode is higher than the bottom of the plated part, so as to avoid the current of the super-long part of the anode being distributed to the plated part and showing a "dog bone" shape, that is, the upper chrome layer is too thick, the thinnest in the middle and thicker in the lower part.


The length of the chrome-plated anode is usually determined according to the depth of the plating tank. Unless a special anode designed and manufactured with a stereotyped product is used, the lower part of the anode is generally about 15 cm from the bottom of the tank, and the upper part is 5 cm above the liquid level. For the anode in this state, if electroplating shaped products (usually shaft parts), the anode surface beyond the plating part (top or bottom) can be encapsulated with plastic tape for insulation; if it is an unshaped product or a workpiece with inconsistent lengths , protective cathodes can be added to the upper and lower parts of the plated parts.


2 Influence of longitudinal distribution of internal resistance


2.1 Solution resistance


The longitudinal distribution state of the solution resistance makes the hydrogen bubbles generated during the chrome plating process overflow from the barrel continuously, which drives the solution to flow from bottom to top and is constantly updated. At this time, the mass concentration of the upper solution is low, and the number of bubbles is large so that the longitudinal distribution of the solution resistance is in an uneven state.


2.2 Polarization resistance


Since the number of bubbles in the plating solution is in a gradient state with more up and down, the more space occupied by the bubbles goes up, the more the exchange rate of the solution in the upper part of the cathode is faster than that in the lower part. The uneven state of the flow rate also causes the longitudinal distribution of the polarization resistance to be a gradient state with a small top and a large bottom.


2.3 Anode resistance


The chrome plating of the barrel is generally made of steel wire with lead-plated anode. The potential drop caused by the resistance of the steel core anode makes the voltage between the cathode and anode different on different sections in the barrel (for example, the voltage on the upper part is higher than that on the lower part), forming a top-to-bottom gradient state. This state makes the longitudinal distribution of the current on the surface of the cathode non-uniform.


3 The effect of trivalent chromium


The mass concentration of trivalent chromium in the chrome plating solution has a significant effect on the longitudinal distribution of internal resistance. Practice has proved that with the increase of the mass concentration of trivalent chromium in the plating solution, the inhomogeneity of the longitudinal distribution of internal resistance is gradually improved. When the mass concentration of trivalent chromium is high, the flow rate of the solution from bottom to top in the barrel becomes slower, which is obviously caused by the slower gas generation rate. The slower the solution flow rate, the larger the mass concentration gradient of the solution, resulting in an increase in the longitudinal gradient of the solution resistance; at the same time, the difference in the alternating rates of the solutions on the upper and lower cathode surfaces is reduced, resulting in a decrease in the longitudinal gradient of the polarization resistance. The increase of the longitudinal gradient of the solution resistance and the decrease of the longitudinal gradient of the polarization resistance are both conducive to the formation of the gradient of the resistance (including the anode resistance) at the top and the bottom, thereby improving the uniformity of the longitudinal distribution of the current.


During the chrome plating process, the basic chromium chromate film is continuously formed on the surface of the cathode, and the chromium sulfate ion is continuously dissolving the basic chromium chromate film in the cathode. The process of film formation and dissolution is carried out alternately on the cathode surface. When the dissolution rate of the film is slow, the hydrogen evolution is faster; when the dissolution rate of the film is faster, the hydrogen evolution is slower. Therefore, it is considered that when the mass concentration of trivalent chromium is high, the number of chromium sulfate ions in the solution increases, which accelerates the dissolution of the basic chromium chromate film on the cathode, thus slowing down the precipitation of hydrogen. It may be because the resistance to be overcome when trivalent chromium is oxidized to hexavalent chromium is smaller than the resistance to be overcome when oxygen is separated out, so when the mass concentration of trivalent chromium increases, the reaction rate of trivalent chromium oxidation to hexavalent chromium is accelerated, Correspondingly, the generation rate of oxygen is suppressed.


In view of this, for the chrome plating of the barrel (especially the slender barrel), the mass concentration of trivalent chromium in the chrome plating solution must be maintained above 10 g/L (the process is specified in the range of 8-12 g/L). When the mass concentration of trivalent chromium is low, the deposition rate of the upper chromium layer is fast and the lower one is slow, forming an uneven chromium plating layer that is thick on the top and thin on the bottom. However, when the mass concentration of trivalent chromium is too high (generally more than 14 g/L), the deposition rate of the upper chromium layer is slow and the lower one is fast, forming an uneven chromium plating layer with a thin top and a thick bottom.


In addition, ferric ions also have an effect, which has a similar effect on the alternate process of film formation and dissolution on the cathode surface and trivalent chromium. That is to say, both ferric ions and trivalent chromium affect the hydrogen generation rate. Therefore, it is stipulated in the process that the mass concentration of ferric ions should be less than 8 g/L.


4 Conclusion


(1) Generally, the uniformity of the thickness of the chrome plating layer depends on the relationship between the anode and the plated parts. Therefore, the spacing between the anode and the plated parts must be reasonably controlled during operation.


(2) The longitudinal taper of the thickness of the chrome plating layer of the gun barrel is closely related to the mass concentration of trivalent chromium in the chrome plating solution. In order to obtain an ideal chromium plating layer, the mass concentration of trivalent chromium should be strictly controlled within a certain range.