sunxinzheng2008@163.com    +86-13713943531
enLanguage
Cont

Have any Questions?

+86-13713943531

Apr 14, 2022

Study on the process and performance of Ni-W plating

Study on the process and performance of Ni-W plating on ABS plastic surface and the mechanism

ABS plastic is light, non-toxic, has good molding processability, high surface finish, good paintability and dyeability, and is easy to be plated. The Ni-W alloy plating has excellent hardness and wear resistance, as well as good appearance and gloss. The Ni-W alloy plating of ABS can greatly improve the hardness and wear resistance of the plated layer and give the ABS surface a metallic lustre, extending the range of applications for ABS plastics. In this paper, Ni-W alloy plating was applied to ABS plastic surface for the first time. The surface of ABS was metallised using degreasing, roughening, sensitisation, ionic activation, chemical copper plating and thickened copper plating successively, and the best process for surface metallisation was determined through experiments. The metallised ABS plastics were alloy plated and the effects of changes in process parameters on the electrodeposition rate and surface hardness of the specimens were investigated by microscopic observation, surface hardness testing, surface morphology determination and bonding force testing; modern material testing techniques such as EDS energy spectral analysis and X-ray diffraction were applied to study the composition and structure of the plated layers and to analyse and study the Ni-W alloy with different W contents in the plated layers The structural forms of Ni-W alloys with different W contents in the plating were investigated. The experimental results and theoretical analysis of ABS plastic surface metallisation show that: 1) Through repeated experiments, the process flow of ABS plastic alloy plating was determined: degreasing, roughening, sensitisation, activation, chemical copper plating to metallise the ABS surface, followed by thickening copper plating and finally electrodeposition of Ni-W alloy plating. 2) Commonly used roughening and activation processes were explored, and the use of a high chromic anhydride type roughening solution and a silver nitrate ion type activation solution was determined, taking into account cost and effectiveness. 3) Experiments were carried out on the chemical copper plating process for the metallisation of plastic surfaces. The effects of chemical copper plating on the ABS plastic substrate were discussed, and the influence of the chemical copper plating parameters on the stability of the plating solution and the adhesion of the plating layer to the substrate was investigated. Based on the experimental results, the chemical copper plating process and process parameters were determined. The experimental results and studies of Ni-W alloy plating show that: 1) as the nickel sulphate content in the plating solution increases, the number of nickel ions in the plating solution increases, more and more nickel ions than hydrogen ions collect on the cathode surface, the hydrogen precipitation reaction decreases, the plating speed and surface hardness increase, and the surface morphology becomes better. As the sodium tungstate content increases, the WO_4~(2-) ions in the solution increase, and the tungsten metal that can be induced to precipitate increases, but the relative Ni~(2+) ion concentration decreases, thus affecting the nickel atom precipitation on the cathode surface and reducing the possibility of tungsten induced precipitation, making the plating speed increase and then decrease; at the same time, as the sodium tungstate increases, the Ni-W solid solution lattice distortion increases and the hardness increases, but when However, when the Ni-W alloy transitions from the nanocrystalline to the amorphous state, the crystals tend to slide and the surface hardness decreases; with too high a sodium tungstate content, the ability of nickel-induced co-deposition is limited, and the presence of too much sodium tungstate is not conducive to the formation of a dense appearance of the plated layer, resulting in a decrease in the morphological quality of the specimen. The influence of citric acid as a complexing agent is mainly reflected in the fact that when its content is low, it cannot meet the need of forming more complexes of metal ions in the plating solution, which affects the plating speed, while sufficient citric acid content is beneficial to the plating effect, too much citric acid will not bring more improvement to the plating effect. 2) The cathode current density has a direct effect on the hardness of the specimen, which is due to the alloy grain growth of the plating layer being influenced by the high plating speed, which develops in the direction of small size, and the surface hardness is thus increased all the time; as the current density increases, the more material precipitates on the electrode surface, the more alloy precipitates on the cathode surface, and the plating speed increases, but the precipitation of hydrogen becomes more and more intense as the current density increases, which hinders the plating speed instead. At the same time, there is an upper limit to the rate of metal deposition and the plating rate tends to stabilise; in addition, the excessive current density makes it too late to replenish the deposited ions consumed in the electrolyte near the cathode, resulting in a decrease in the quality of the specimen's appearance. 3) The influence of the pH of the plating solution on the surface morphology of the specimen is more direct than other conditions. 4) The increase in temperature of the plating solution enhances the diffusion ability of metal ions and increases the concentration of metal ions in the cathode diffusion layer, which not only facilitates the acceleration of the plating speed, but also facilitates the refinement of Ni-W grains and surface densification, and improves the surface hardness and appearance of the morphology, but the high temperature causes the decomposition and volatilization of the complexing agent and additives, and the plating solution becomes unstable, which adversely affects the plating speed, surface hardness and morphology of the specimens. 5) The Ni-W plating was tested by XRD and the observations and calculations proved that the Ni-W alloy in the plating was a replacement solid solution with Ni as the solvent and W as the solute, and the grain size was between 20 and 40 nm, and the plating was a nanocrystalline plating, while with the increase of W content, the Ni-W alloy structure gradually changed to the amorphous state, and when the W content was 45.56%, the Ni-W alloy plating was The Ni-W alloy layer was amorphous when the W content was 45.56%. 6) The results of the orthogonal experiments showed that: the content ratio of nickel sulphate/sodium tungstate had the greatest influence on the surface hardness of the specimen, and had a considerable influence on the wear resistance and surface morphology; the influence of the temperature of the plating solution on the surface hardness, wear resistance and surface morphology was the smallest among the four factors; the pH value of the plating solution had the most significant influence on the wear resistance, and also had a greater influence on the surface hardness, while the influence on the surface morphology was smaller. The influence of cathodic current density on surface hardness and wear resistance is greater, while the influence on surface morphology is less significant. 7) The optimum Ni-W alloy plating formula was optimised by orthogonal tests: 60g/L nickel sulphate, 150g/L sodium tungstate, 130g/L citric acid, 65°C plating solution temperature, pH 5, 20A/dm~2 current density and 30min plating time. The Ni-W alloy plating has a relative abrasion resistance of 4.2. The bonding test results show that the plating is well bonded to the substrate, and the plating has a fine and flat appearance with a high gloss.


Send Inquiry