Solutions to nine common faults of plastic electroplating-nickel plating.
Huizhou Boluo Tenglong Technology Co., Ltd. serves you wholeheartedly! Mainly engaged in plastic hydroelectroplating processing, with plastic injection molding processing, mold processing and so on!
The main disadvantages of nickel plating are: poor pretreatment, metal impurities, too little boric acid content, too low bath temperature will lead to pinholes in the nickel plating layer, and bath maintenance and strict control of the process is the key. If the following "nine" major failures are solved, the basic problems will be brought under control.
1) Ma Keng (pinhole).
Ma Keng (pinhole) is the result of organic pollution. Large pockholes usually indicate that there is oil pollution to decompose oil carbon treatment. If the mixing is poor, the bubbles cannot be expelled, and pockmarked holes (pinholes) can be formed. Wetting agents can be used to reduce their effects.
2) rough (burr).
Roughness means that the solution dirty after full filtration can be corrected too high and easy to form hydroxide precipitation, which should be controlled; when the current density is too high, anode mud and added water are impure with human impurities, roughness (burr) will be produced in serious cases.
3) low binding force.
If the copper coating is not activated to remove the oxide layer, the adhesion between copper and nickel is poor, the coating will peel off. If the current is interrupted, it may cause the nickel coating to peel off itself; if the temperature is too low, it will also peel off.
4) brittleness and poor solderability of the coating.
When the coating is bent or worn to a certain extent, the brittleness of the coating is usually revealed, which indicates the existence of organic or heavy metal pollution. Too many additives increase the organic matter and decomposition products in the coating, which is the main source of organic pollution and can be treated with activated carbon, and heavy metal impurities can be removed by electrolysis.
5) the coating is dark and uneven in color.
The darkening and uneven color of the coating indicate metal contamination. Because copper plating is usually followed by nickel plating, the copper solution is the main source of pollution. It is important to minimize the copper solution in the hanger. In order to eliminate the metal pollution in the nickel plating bath, the corrugated steel plate is used as the cathode and electrolyzed at the current density of 02-0.5A/dm2. Poor pretreatment, poor bottom coating, low current density, low concentration of main salt and poor conductive contact will affect the color of the coating.
6) Coke coating.
Insufficient boric acid, low concentration of metal salts, too low working temperature, too high current density, too high PH value or insufficient stirring are all possible causes of coke burning of the coating.
7) low deposition rate or low current density will lead to low deposition rate.
8) blistering or peeling of the coating.
Blistering or peeling will occur when poor pre-plating treatment, long power cut-off time, organic impurity pollution, too high current density, too low temperature, too high or too low PH value, and serious influence of impurities will occur.
9) Anodic passivation.
Insufficient anodic activator (nickel chloride), too small anode area and too high current density will lead to anode passivation.