Plastic plating-Ni-SiC composite coating on ABS plastic grinding head

Plastic plating-Ni-SiC composite coating on ABS plastic grinding head.
Huizhou Boluo Tenglong Technology Co., Ltd. serves you wholeheartedly! Mainly engaged in plastic hydroelectroplating processing, with plastic injection molding processing, mold processing and so on!
ABS plastic is a terpolymer of acrylonitrile, butadiene and styrene. It has the characteristics of ordinary plastic. Electroplating Ni-SiC composite coating on AB S plastic grinding head can combine its light weight, easy machining and high hardness and strong grinding force of SiC particles. To achieve this, we must first metallize the plastic surface so that it can conduct electricity, and then plating Ni-SiC composite coating on the surface.
1 technological process.
Electroplating Ni-SiC composite coating on ABS plastic grinding head. The technological process is as follows: ABS plastic grinding head "de-stress", "deoiling", "coarsening", "water washing" and "water washing" primary reduction "washing", "pickling", washing "sensitizing", "washing" deionizing, "activation", "washing", secondary reduction "washing", "electroless copper plating", "water washing", "weak erosion", "copper plating", "water washing", pre-plating nickel "Ni-SiC composite plating" bright nickel "water washing" Hot water washing "unhanger"dry" surface dressing "quality inspection package."
2 description of the main process.
The main results are as follows: (1) the ABS plastic grinding head is soaked in 25% acetone for about 30 min to eliminate the internal stress of ABS plastic grinding head.
The purpose of copper plating is to thicken the copper coating. Because the expansion coefficient of copper is close to that of ABS plastic, thickening copper coating can reduce the effect of temperature change on the adhesion between plastic substrate and coating.

3 points for attention.
Insufficient or excessive coarsening will reduce the adhesion of the coating. The lack of coarsening is also easy to expose the plastic matrix, and excessive coarsening of plastics is easy to produce cracks. Coarsening temperature should not be too high, generally should be less than 60 ℃, so as to avoid plastic grinding head deformation.
When electroplating, the nickel anode must use the anode sleeve, and often clean the anode mud to prevent the anode mud from forming nickel tumor on the surface of the grinding head. If the anode sleeve is damaged and the anode mud is mixed into the plating bath, a magnet can be used to remove it.
Lower current density is suitable for Ni-SiC composite plating. Because the SiC particles do not conduct electricity, the actual surface area of the grinding head is lower than the macroscopic surface area. If the current density is too high, a large amount of hydrogen will be precipitated, which may disperse the SiC particles covered by the surface, and it is easy to make the pH value of the plating solution on the surface of the grinding head rise sharply and form nickel hydroxide precipitation, resulting in the decline of the quality of the coating.
The thickness of the coating should be equal to the particle size of SiC particles. It is necessary not only to make the particles firmly fixed in the coating, but also to prevent the coating from overwrapping the particles and make them lose their grinding effect.
4 knot theory.
The adhesion test of the coating was carried out according to GB/ T 12610. The test period was 4 thermal cycles. After the test, the coating did not appear blistering, cracking, shedding and so on. The mass fraction of SiC measured by gravimetric method is 20%. This process expands the application range of ABS plastics and has great practical value. Tens of thousands of sets of qualified products have been successfully processed for a foreign enterprise, and good economic benefits have been achieved.

Send Inquiry