Common Faults Of ABS Plastic Plating

Plastic plating-Common faults of ABS plastic plating.
Huizhou Boluo Tenglong Technology Co., Ltd. serves you wholeheartedly! Mainly engaged in plastic hydroelectroplating processing, with plastic injection molding processing, mold processing and so on! .
In order to obtain a perfect coating for ABS plastic plating, efforts must be made on a series of factors, such as mold design, manufacture, selection of ABS plastics, injection molding and so on. This paper mainly gives the troubleshooting methods of common faults from the point of view of chemical plating and electroplating.

(1) the deposition of electroless coating is incomplete. The deposition of regular fixed site is not all the manifestation of internal stress concentration. The products should be de-stressed. Irregular and random deposition incompleteness should be found first from coarsening, then insufficient activation, and finally the decline of electroless plating efficiency, which should be corrected according to the reasons found.
t01ebe9f1a9145bdd01
(2) peeling of electroless coating together with electroless coating. If the coarsening is insufficient, it is common to see that the electroless coating is bright and the local fixed part is peeled, which belongs to the concentration point of internal stress. Coarsening and stress relief should be strengthened.

(3) peeling between coatings. Bright coating, especially bright nickel plating, has high internal stress, which may lead to brightener maladjustment. It is also possible that the pH of nickel plating is too high or the oxidation or passivation of the intermediate coating leads to poor adhesion of the surface coating. Adjust the plating bath and pay attention to strengthening the activation of the intermediate coating. Change the activation fluid frequently. During chromium plating, the parts stay preheated in the bath for a while and then turn on electroplating.
t0147c32c8f64b83c12
(4) the coating dissolves locally in the product. The electrical conductivity of the hanger is poor, resulting in a "bipolar" phenomenon, which makes the part become an anode and dissolve. Pay attention to the hanger and parts must have more than two contacts, and must ensure good contact.

There are burrs and spots on the 5ABS coating. The deposition of physical impurities on the surface caused by the dirty plating bath may also be caused by the influence of copper powder and nickel plating anode slime. The plating bath should be filtered regularly. All anodes should be protected by anode bags. Do not salvage the parts or stir the plating solution from the bottom in the production process. Usually cover it when you don't use the plating solution.

The occurrence of pitting is mostly due to the low pH value of bright nickel plating, which aggravates hydrogen evolution and the lack of surfactants. Adjust the pH value of the bath to the normal range and add surfactants such as sodium dodecyl sulfate to reduce the adsorption of hydrogen.

(6) the parts are deformed after plating. After the completion of ABS plastic plating, it is sometimes found that some products are deformed, affecting the assembly or use. For example, the outer frame, shell, nameplate, matching components, etc., if there is deformation, there will be no method to install and use.

There are three reasons for this quality problem. One is that the design itself is unreasonable and there are design defects. The other is that the design of the hanger is unreasonable. Also, the process control is not strict and the operation is improper.

Mold design should pay full attention to the relationship between product thickness and shrinkage, and consider the strength requirements. Where it is too thin, there should be reinforcement and strain tendons to offset the stress. As the strength increases, so does the resistance to deformation.
t0166e9c4250b429554
The fulcrum of the hanger should be symmetrically set, and maintain the same tension, the tension of the hanger is unbalanced, it will be deformed after a higher temperature process, and the deformation will be fixed after cooling. Therefore, the design and production of the hanger should be reasonable. Do not force the plated parts too much in a certain direction, you can increase the fulcrum contact surface and reduce the fulcrum tension.

In the operation, strictly according to the process requirements to manage each process, do not exceed the prescribed temperature. In the process of electroplating, it is found that the individual fulcrum shedding should be corrected to avoid uneven force and deformation of the products. In particular, it is necessary to strengthen the management of the drying oven and often check whether the constant temperature control equipment is in an effective state. And often use an accurate mercury thermometer to check the oven temperature shown in the figures. Pay attention to the temperature monitoring of the process with heating requirements, such as coarsening, bright nickel plating, chromium plating, etc.

 