Plastic Electroplating-ABS Plastic Copper Plating Process

Plastic Electroplating-ABS Plastic Copper Plating Process

Plastic Electroplating-ABS plastic Copper plating process. Huizhou Boluo Tenglong Technology Co., Ltd. serves you wholeheartedly! Mainly engaged in plastic hydroelectroplating processing, with plastic injection molding processing, mold processing and so on! The process of plastic electroplating...
Send Inquiry

Product Introduction

Plastic Electroplating-ABS plastic Copper plating process.
Huizhou Boluo Tenglong Technology Co., Ltd. serves you wholeheartedly! Mainly engaged in plastic hydroelectroplating processing, with plastic injection molding processing, mold processing and so on!
The process of plastic electroplating is as follows:
De-stress "stress inspection" chemical deoiling "coarsening" reduction "sensitization" activation "secondary reduction" electroless copper plating "electroplating copper" test.

t01416fe9f5dbcae845
1.2.2 Operation points of each process.
1) de-stress. The sample was treated in a thermostat at 80 ℃ for 8 h.
2) stress inspection. Soak the sample in glacial acetic acid, 3min, clean the surface and dry. Observe the surface under a 40x metallographic microscope to ensure that there are no cracks.
3) Chemical oil removal. 5g/L Sodium hydroxide, 20g/L Sodium Carbonate, 20g/L Sodium Phosphate, 1g/L Sodium dodecyl Sulfonate, θ is 60-65 ℃, t is 30min.

t01394364d7fd077433
4) coarsening. 400g/L chromic anhydride, 400g/L concentrated sulfuric acid, θ is 70 ℃ 75 ℃, t is 25~30min.
5) restore. 50g/L sodium hydroxide, room temperature, t is 5min.
6) sensitization. 10g/L stannous chloride, 70mL/L concentrated hydrochloric acid, room temperature, t is 3min.
7) Activation. 2g/L silver nitrate, 150mL/L ammonia, room temperature, t is 5min.
8) second reduction. 1g/L sodium hydroxide, 1g/L potassium borohydride, room temperature, t is 2min.
9) Electroless copper plating. Solution A: 8g/L copper sulfate, 27g/L potassium hydrogen tartrate, 23g/L sodium hydroxide, 0.3g point L2-mercaptobenzothiazole, 4g/L ammonium chloride; solution B: v (Glyoxal): v (water) = 1:4. V (solution A): v (solution B) = 3:1, room temperature, t = 30min pH 10.9.
10) Copper plating. 50g/L basic copper carbonate, 250g/L citric acid, 30g/L potassium sodium tartrate, 10g/L sodium bicarbonate, pH=8. The anode is phosphorus copper plate, J is 1.0A/dm2, room temperature, t is 30min.

 

Hot Tags: plastic electroplating-abs plastic copper plating process, China, suppliers, manufacturers, factory, custom, wholesale, buy, made in China